EN 10113-2 is the standard Hot Rolled Product in Weldable Fine Grain Structural Steel in delivery condition of Normalized or Normalized rolled .
S275N , S275NL, S355NL1, S355NL , S420N, S420NL,S460N,S460NL steel Chemical composition % max :
Grade |
C |
Si |
Mn |
P |
S |
Nb |
V |
Al |
Ti |
Cr |
Ni |
Mo |
Cu |
N |
S275N |
0.18 |
0.40 |
0.5-1.40 |
0.035 |
0.030 |
0.05 |
0.05 |
0.02 |
0.03 |
0.30 |
0.30 |
0.10 |
0.35 |
0.015 |
S275NL |
0.16 |
0.030 |
0.025 |
|||||||||||
S355N |
0.20 |
0.50 |
0.9-1.65 |
0.035 |
0.030 |
0.05 |
0.12 |
0.02 |
0.03 |
0.30 |
0.50 |
0.10 |
0.35 |
0.015 |
S355NL |
0.18 |
0.030 |
0.025 |
|||||||||||
S420N |
0.20 |
0.60 |
1.0-1.70 |
0.035 |
0.030 |
0.05 |
0.20 |
0.02 |
0.03 |
0.30 |
0.80 |
0.10 |
0.70 |
0.025 |
S420NL |
0.030 |
0.025 |
||||||||||||
S460N |
0.20 |
0.60 |
1.0-1.70 |
0.035 |
0.030 |
0.05 |
0.20 |
0.02 |
0.03 |
0.30 |
0.80 |
0.10 |
0.70 |
0.025 |
S460NL |
0.030 |
0.025 |
S275N , S275NL, S355NL1, S355NL , S420N, S420NL,S460N,S460NL steel steel Mechanical properties at ambient temperature for normalized steel.
Grade |
Tensile Strength N/mm2 |
Yield Strength in mm (MPa min) |
EL % min. |
||||||
|
≤100mm |
>100mm |
≤16 |
>16 |
>40 |
>63 |
>80 |
>100 |
|
S275N |
370-150 |
350-480 |
275 |
265 |
255 |
245 |
235 |
225 |
24 |
S275NL |
|||||||||
S355N |
470-630 |
450-600 |
355 |
345 |
335 |
325 |
315 |
295 |
22 |
S355NL |
|||||||||
S420N |
520-680 |
500-660 |
420 |
400 |
390 |
370 |
360 |
340 |
19 |
S420NL |
|||||||||
S460N |
550-720 |
- |
460 |
440 |
430 |
410 |
400 |
- |
17 |
S460NL |